Typically, CN was synthesized by calcining melamine powder (10 g) at 550 °C for 4 h with a ramping rate of 5 °C min−1 in static air in a muffle furnace. After naturally cooling down to room temperature, the resulting product was dissolved into 0.5 M HNO3 solution, bathing for 4 h at 80 °C. Then, light yellow agglomerates were gathered, cross-washed with deionized water and ethanol several times, and dried at 60 °C in a vacuum oven for further use.